Minerals - Densities
Densities of some common minerals:
| Mineral | Comment | Density (ranging from to) | |||||
|---|---|---|---|---|---|---|---|
| (g/cm3) | (kg/m3) | (lb/ft3) | |||||
| Acanthite | 7.2 | 7.3 | 7200 | 7300 | 449 | 456 | |
| Acmite | Pyroxene group | 3.52 | 3520 | 220 | |||
| Actinolite | Amphibole group | 3.04 | 3040 | 190 | |||
| Alabandite | 4 | 4000 | 250 | ||||
| Alamandine | Garnet group | 4.09 | 4.31 | 4090 | 4310 | 255 | 269 |
| Albite | Feldspar | 2.62 | 2620 | 163 | |||
| Allanite | 3.3 | 4.2 | 3300 | 4200 | 206 | 262 | |
| Allemontite | 6.15 | 6150 | 384 | ||||
| Allophane | Clay group or clay like | 1.9 | 1900 | 119 | |||
| Altaite | 8.14 | 8140 | 508 | ||||
| Alunite | 2.59 | 2.9 | 2590 | 2900 | 162 | 181 | |
| Amblygonite | 2.98 | 3.11 | 2980 | 3110 | 186 | 194 | |
| Analcime | 2.3 | 2300 | 144 | ||||
| Anatese | 3.9 | 3900 | 243 | ||||
| Andalusite | 3.15 | 3150 | 197 | ||||
| Andesine | Pyroxene group | 2.67 | 2670 | 167 | |||
| Andradite | Garnet group | 3.7 | 4.1 | 3700 | 4100 | 231 | 256 |
| Anglesite | 6.3 | 6300 | 393 | ||||
| Ankerite | Carbonate group | 3.05 | 3050 | 190 | |||
| Annebergite | 3.05 | 3050 | 190 | ||||
| Anorthite | 2.73 | 2730 | 170 | ||||
| Anorthoclase | Orthoclase | 2.58 | 2580 | 161 | |||
| Anthophyllite | Amphibole group | 2.85 | 3.57 | 2850 | 3570 | 178 | 223 |
| Anthydrite | 2.97 | 2970 | 185 | ||||
| Antimony | 6.66 | 6660 | 416 | ||||
| Antlerite | 3.9 | 3900 | 243 | ||||
| Apatite | 3.19 | 3190 | 199 | ||||
| Apidote | 3.3 | 3.6 | 3300 | 3600 | 206 | 225 | |
| Apophyllite | 2.34 | 2340 | 146 | ||||
| Aragonite | 2.93 | 2930 | 183 | ||||
| Arfvedsonite | Amphibole group | 3.44 | 3440 | 215 | |||
| Argenite | 7.3 | 7300 | 456 | ||||
| Arsenic | 5.7 | 5700 | 356 | ||||
| Arsenopyrite | 6.07 | 6070 | 379 | ||||
| Atacamite | 3.76 | 3760 | 235 | ||||
| Augite | 3.4 | 3400 | 212 | ||||
| Aurichalcite | 3.64 | 3.9 | 3640 | 3900 | 227 | 243 | |
| Autonite | 3.15 | 3150 | 197 | ||||
| Awaruite | 8 | 8000 | 499 | ||||
| Axinite | 3.28 | 3280 | 205 | ||||
| Azurite | 3.83 | 3830 | 239 | ||||
| Barite | 4.48 | 4480 | 280 | ||||
| Bastnaesite | Rare earth oxide group | 4.95 | 4950 | 309 | |||
| Beidellite | Clay group or clay like | 2.15 | 2150 | 134 | |||
| Beryl | 2.63 | 2.9 | 2630 | 2900 | 164 | 181 | |
| Biotite | Mica group | 2.8 | 3.5 | 2800 | 3500 | 175 | 218 |
| Bismite | 8.5 | 9.5 | 8500 | 9500 | 530 | 593 | |
| Bismuth | 9.75 | 9750 | 608 | ||||
| Boehmite | Bauxite component | 3.03 | 3030 | 189 | |||
| Boracite | 2.9 | 2900 | 181 | ||||
| Borax | 1.71 | 1710 | 107 | ||||
| Bornite | 5.09 | 5090 | 318 | ||||
| Boulangerite | 5.7 | 6.3 | 5700 | 6300 | 356 | 393 | |
| Brannerite | 4.5 | 6.5 | 4500 | 6500 | 281 | 406 | |
| Braunite | 4.76 | 4760 | 297 | ||||
| Bravoite | 5.01 | 5010 | 313 | ||||
| Brochantite | 3.97 | 3970 | 248 | ||||
| Bromargyrite | 5.8 | 6 | 5800 | 6000 | 362 | 374 | |
| Bronzite | Enstatite group | 3.2 | 3.9 | 3200 | 3900 | 200 | 243 |
| Brookite | 4.11 | 4110 | 256 | ||||
| Brucite | 2.39 | 2390 | 149 | ||||
| Bytownite | Plagioclase group | 2.71 | 2710 | 169 | |||
| Calcite | 2.71 | 2710 | 169 | ||||
| Calomel | 6.45 | 6450 | 402 | ||||
| Calvarite | 9.04 | 9040 | 564 | ||||
| Cancrinite | Feldspathoid group | 2.45 | 2450 | 153 | |||
| Carnallite | 1.6 | 1600 | 100 | ||||
| Carnotite | 3.7 | 4.7 | 3700 | 4700 | 231 | 293 | |
| Cassiterite | 6.9 | 6900 | 431 | ||||
| Celestite | 3.95 | 3950 | 246 | ||||
| Celsian | Feldspar group | 3.25 | 3250 | 203 | |||
| Cerargyrite | 5.55 | 5550 | 346 | ||||
| Cerussite | Carbonate group | 6.58 | 6580 | 411 | |||
| Cervanite | 6.5 | 6500 | 406 | ||||
| Chabazite | Zeolite group | 2.09 | 2090 | 130 | |||
| Chalcanthite | 2.21 | 2210 | 138 | ||||
| Chalcocite | 5.5 | 5.8 | 5500 | 5800 | 343 | 362 | |
| Chalcopyrite | 4.19 | 4190 | 261 | ||||
| Chlorite | 2.42 | 2420 | 151 | ||||
| Chloritoid | Mica group | 3.51 | 3.8 | 3510 | 3800 | 219 | 237 |
| Chondrodite | 3.15 | 3150 | 197 | ||||
| Chromite | 4.5 | 5.09 | 4500 | 5090 | 281 | 318 | |
| Chrysoberyl | 3.5 | 3.84 | 3500 | 3840 | 218 | 240 | |
| Chrysocolla | 2 | 2.4 | 2000 | 2400 | 125 | 150 | |
| Cinnibar | 8.1 | 8100 | 505 | ||||
| Clinochlore | 2.65 | 2650 | 165 | ||||
| Clinoclase | 4.29 | 4290 | 268 | ||||
| Clinoenstatite | Enstatite group | 3.4 | 3400 | 212 | |||
| Clinoferrosilite | Enstatite group | 4.1 | 4100 | 256 | |||
| Clinohumite | 3.26 | 3260 | 203 | ||||
| Clinzoite | 3.34 | 3340 | 208 | ||||
| Cobaltite | 6.33 | 6330 | 395 | ||||
| Colemanite | 2.42 | 2420 | 151 | ||||
| Columbite | 5.3 | 7.3 | 5300 | 7300 | 331 | 456 | |
| Copper | 8.94 | 8940 | 558 | ||||
| Cordierite | 2.55 | 2.77 | 2550 | 2770 | 159 | 173 | |
| Corundum | 4.05 | 4050 | 253 | ||||
| Coveillite | 4.68 | 4680 | 292 | ||||
| Cristobalite | 2.27 | 2270 | 142 | ||||
| Crocoite | 6 | 6000 | 374 | ||||
| Cryolite | 2.97 | 2970 | 185 | ||||
| Cubanite | 4.7 | 4700 | 293 | ||||
| Cummingtonite | Amphibole group | 3.35 | 3350 | 209 | |||
| Cuprite | 6.1 | 6100 | 381 | ||||
| Danburite | 2.99 | 2990 | 187 | ||||
| Datolite | 2.9 | 2900 | 181 | ||||
| Diamond | 3.51 | 3510 | 219 | ||||
| Diaspore | 3.4 | 3400 | 212 | ||||
| Dickite | Clay group or clay like | 2.6 | 2600 | 162 | |||
| Digenite | 5.6 | 5600 | 349 | ||||
| Diopside | Pyroxene group | 3.4 | 3400 | 212 | |||
| Dioptase | 3.31 | 3310 | 207 | ||||
| Dolmite | Carbonate group | 2.84 | 2840 | 177 | |||
| Dumortierite | 3.34 | 3340 | 208 | ||||
| Edenite | Hornblende | 3.02 | 3020 | 188 | |||
| Embolite | 5.6 | 5600 | 349 | ||||
| Enargite | 4.45 | 4450 | 278 | ||||
| Enstatite | Pyroxene group | 3.2 | 3200 | 200 | |||
| Erythrite | 3.12 | 3120 | 195 | ||||
| Espomite | 1.67 | 1670 | 104 | ||||
| Euclase | 3.04 | 3040 | 190 | ||||
| Euxenite | 4.84 | 4840 | 302 | ||||
| Fayalite | Olivine group | 4.39 | 4390 | 274 | |||
| Feberite | 7.45 | 7450 | 465 | ||||
| Fergusonite | Rare earth oxide group | 4.5 | 5.7 | 4500 | 5700 | 281 | 356 |
| Ferrimolybdite | 4 | 4.5 | 4000 | 4500 | 250 | 281 | |
| Ferrosilite | Pyroxene group | 3.95 | 3950 | 246 | |||
| Fluorite | 3.13 | 3130 | 195 | ||||
| Forsterite | Olivine group | 3.27 | 3270 | 204 | |||
| Franklinite | 5.14 | 5140 | 321 | ||||
| Gadolinite | Rare earth oxide group | 4 | 4.5 | 4000 | 4500 | 250 | 281 |
| Gahnite | Spinel group | 4 | 4.6 | 4000 | 4600 | 250 | 287 |
| Galaxite | Spinel group | 4.23 | 4230 | 264 | |||
| Galena | 7.2 | 7.6 | 7200 | 7600 | 449 | 474 | |
| Garnierite | 2.41 | 2410 | 150 | ||||
| Gaylussite | 1.96 | 1960 | 122 | ||||
| Geocronite | 6.4 | 6400 | 399 | ||||
| Gersdorffite | 6.11 | 6110 | 381 | ||||
| Gibbsite | 2.34 | 2340 | 146 | ||||
| Glauberite | 2.77 | 2770 | 173 | ||||
| Glauconite | Mica group | 2.4 | 2.95 | 2400 | 2950 | 150 | 184 |
| Glaucophane | Amphibole group | 3.07 | 3070 | 192 | |||
| Gmelinite | Zeolite group | 2.09 | 2090 | 130 | |||
| Goethite | 3.3 | 4.3 | 3300 | 4300 | 206 | 268 | |
| Gold | 19.32 | 19320 | 1206 | ||||
| Goslarite | 2 | 2000 | 125 | ||||
| Graphite | 2.16 | 2160 | 135 | ||||
| Greenocktite | 3.98 | 5 | 3980 | 5000 | 248 | 312 | |
| Grossularite | Garnet group | 3.42 | 3.72 | 3420 | 3720 | 213 | 232 |
| Gypsum | 2.3 | 2300 | 144 | ||||
| Halite | 2.17 | 2170 | 135 | ||||
| Halloysite | Clay group or clay like | 2 | 2.6 | 2000 | 2600 | 125 | 162 |
| Harmotome | 2.46 | 2460 | 154 | ||||
| Hastingsite | Hornblende | 3.17 | 3.59 | 3170 | 3590 | 198 | 224 |
| Hausmanite | 4.76 | 4760 | 297 | ||||
| Hauynite | Feldspathoid group | 2.45 | 2450 | 153 | |||
| Hectorite | Clay group or clay like | 2 | 3 | 2000 | 3000 | 125 | 187 |
| Hedenbergite | 3.55 | 3550 | 222 | ||||
| Helvite | 3.26 | 3260 | 203 | ||||
| Hemimorphite | 3.45 | 3450 | 215 | ||||
| Hercynite | Spinel group | 3.95 | 3950 | 246 | |||
| Hermatite | 5.3 | 5300 | 331 | ||||
| Hessite | 7.2 | 7.9 | 7200 | 7900 | 449 | 493 | |
| Heulandite | 2.2 | 2200 | 137 | ||||
| Hornblende | Hornblende | 3 | 3.47 | 3000 | 3470 | 187 | 217 |
| Huebnerite | Wolframite series | 7.15 | 7150 | 446 | |||
| Humite | 3.15 | 3150 | 197 | ||||
| Hyalophane | Orthoclase | 2.81 | 2810 | 175 | |||
| Hydrozincite | 3.2 | 3.8 | 3200 | 3800 | 200 | 237 | |
| Hypersthene | Hornblende | 3.2 | 3.9 | 3200 | 3900 | 200 | 243 |
| Ice | 0.99 | 990 | 62 | ||||
| Iddingsite | 2.5 | 2.8 | 2500 | 2800 | 156 | 175 | |
| Idocrase | 3.4 | 3400 | 212 | ||||
| Illemenite | 4.72 | 4720 | 295 | ||||
| Illite | Clay group or clay like | 2.6 | 2.9 | 2600 | 2900 | 162 | 181 |
| Ilvaite | 4.01 | 4010 | 250 | ||||
| Iodobromite | 5.7 | 5700 | 356 | ||||
| Iodyrite | 5.6 | 5600 | 349 | ||||
| Irdosmine | 19.3 | 21 | 19300 | 21000 | 1204 | 1310 | |
| Iridium | 22.7 | 22700 | 1416 | ||||
| Jacobsite | Spinel group | 4.75 | 4750 | 296 | |||
| Jadeite | Pyroxene group | 3.3 | 3300 | 206 | |||
| Jamesonite | Jamesonite group | 5.56 | 5560 | 347 | |||
| Jarosite | 2.9 | 3.3 | 2900 | 3300 | 181 | 206 | |
| Kainite | 2.1 | 2100 | 131 | ||||
| Kaliophilite | 2.58 | 2580 | 161 | ||||
| Kaolinite | Clay group or clay like | 2.6 | 2600 | 162 | |||
| Kernite | 1.91 | 1910 | 119 | ||||
| Krennerite | 8.53 | 8530 | 532 | ||||
| Kyanite | 3.61 | 3610 | 225 | ||||
| Langbeinite | 2.83 | 2830 | 177 | ||||
| Larsenite | Olivine group | 5.9 | 5900 | 368 | |||
| Laumonite | Zeolite group | 2.29 | 2290 | 143 | |||
| Lawsonite | 3.09 | 3090 | 193 | ||||
| Lazulite | 3.05 | 3050 | 190 | ||||
| Lazurite | 2.4 | 2400 | 150 | ||||
| Lechatelierite | 2.5 | 2.65 | 2500 | 2650 | 156 | 165 | |
| Lepidocrocite | 4 | 4000 | 250 | ||||
| Lepidolite | Mica group | 2.84 | 2840 | 177 | |||
| Leucite | Feldspathoid group | 2.47 | 2470 | 154 | |||
| Liebthenite | 3.8 | 3800 | 237 | ||||
| Limonite | 3.3 | 4 | 3300 | 4000 | 206 | 250 | |
| Linarite | 5.4 | 5400 | 337 | ||||
| Linneaeite | 4.8 | 4800 | 300 | ||||
| Lithiophilite | 3.34 | 3340 | 208 | ||||
| Loellingite | 7.1 | 7.4 | 7100 | 7400 | 443 | 462 | |
| Magnesite | Carbonate group | 3 | 3000 | 187 | |||
| Magnetite | 5.15 | 5150 | 321 | ||||
| Malachite | 3.6 | 4 | 3600 | 4000 | 225 | 250 | |
| Manganite | 4.34 | 4340 | 271 | ||||
| Manganosite | 5.18 | 5180 | 323 | ||||
| Marcasite | 4.89 | 4890 | 305 | ||||
| Margarite | Mica group | 3.03 | 3030 | 189 | |||
| Marialite | Scapolite series | 2.56 | 2560 | 160 | |||
| Meionite | Scapolite series | 2.69 | 2690 | 168 | |||
| Melanterite | 1.89 | 1890 | 118 | ||||
| Melilite | 2.95 | 2950 | 184 | ||||
| Menaghinite | Jamesonite group | 6.38 | 6380 | 398 | |||
| Miargyrite | 5.19 | 5190 | 324 | ||||
| Microcline | Feldspar group | 2.56 | 2560 | 160 | |||
| Microlite | 4.2 | 6.4 | 4200 | 6400 | 262 | 399 | |
| Millerite | 5.5 | 5500 | 343 | ||||
| Mimetite | 7.17 | 7170 | 447 | ||||
| Minium | 8.2 | 8200 | 512 | ||||
| Molybdenite | 5.5 | 5500 | 343 | ||||
| Monazite | 4.8 | 5.5 | 4800 | 5500 | 300 | 343 | |
| Monticellite | Olivine group | 3.2 | 3200 | 200 | |||
| Montmotillonite | Clay group or clay like | 2 | 2.7 | 2000 | 2700 | 125 | 168 |
| Mullite | 3.05 | 3050 | 190 | ||||
| Musscovite | Mica group | 2.82 | 2820 | 176 | |||
| Nacrite | Clay group or clay like | 2.6 | 2600 | 162 | |||
| Nagyagite | 7.5 | 7500 | 468 | ||||
| Natrolite | Zeolite group | 2.25 | 2250 | 140 | |||
| Nephheline | 2.55 | 2.65 | 2550 | 2650 | 159 | 165 | |
| Ni skutterudite | 6.5 | 6500 | 406 | ||||
| Niccolite | 7.79 | 7790 | 486 | ||||
| Nitre | 2.1 | 2100 | 131 | ||||
| Nontronite | Clay group or clay like | 2.3 | 2300 | 144 | |||
| Norbergite | 3.15 | 3150 | 197 | ||||
| Noselite | Feldspathoid group | 2.34 | 2340 | 146 | |||
| Oligoclase | 2.65 | 2650 | 165 | ||||
| Opal | 2.09 | 2090 | 130 | ||||
| Orpiment | 3.52 | 3520 | 220 | ||||
| Orthoclase | Feldspar group | 2.56 | 2560 | 160 | |||
| Ottrelite | Mica group | 3.52 | 3520 | 220 | |||
| Palladium | 11.55 | 11550 | 721 | ||||
| Paragonite | Mica group | 2.78 | 2780 | 173 | |||
| Pargasite | Hornblende | 3.12 | 3120 | 195 | |||
| Pearceite | 6.13 | 6130 | 383 | ||||
| Pectolite | 2.86 | 2860 | 178 | ||||
| Pentlandite | 4.6 | 5 | 4600 | 5000 | 287 | 312 | |
| Perovskite | 4 | 4000 | 250 | ||||
| Petalite | Feldspathoid group | 2.42 | 2420 | 151 | |||
| Petzite | 8.7 | 9.14 | 8700 | 9140 | 543 | 570 | |
| Phenaktite | 2.98 | 2980 | 186 | ||||
| Phillipsite | Zeolite group | 2.2 | 2200 | 137 | |||
| Phlogopite | Mica group | 2.7 | 2.9 | 2700 | 2900 | 168 | 181 |
| Phosgenite | 6 | 6.3 | 6000 | 6300 | 374 | 393 | |
| Phosphuranylite | 4.1 | 4100 | 256 | ||||
| Pigeonite | Pyroxene group | 3.3 | 3.46 | 3300 | 3460 | 206 | 216 |
| Plagionite | Jamesonite group | 5.4 | 5.6 | 5400 | 5600 | 337 | 349 |
| Platinum | 21.45 | 21450 | 1339 | ||||
| Polucite | 2.9 | 2900 | 181 | ||||
| Polybasite | 4.6 | 5 | 4600 | 5000 | 287 | 312 | |
| Polycrase | Rare earth oxide group | 5 | 5000 | 312 | |||
| Polyhalite | 2.77 | 2770 | 173 | ||||
| Potash alum | 1.75 | 1750 | 109 | ||||
| Powellite | 4.34 | 4340 | 271 | ||||
| Prehnite | 2.87 | 2870 | 179 | ||||
| Proustite | 5.55 | 5550 | 346 | ||||
| Pyrargyrite | 5.85 | 5850 | 365 | ||||
| Pyrite | 5.01 | 5010 | 313 | ||||
| Pyrochlore | 4.2 | 6.4 | 4200 | 6400 | 262 | 399 | |
| Pyrolusite | 4.4 | 5.06 | 4400 | 5060 | 275 | 316 | |
| Pyromorphite | 6.7 | 7 | 6700 | 7000 | 418 | 437 | |
| Pyrope | Garnet group | 3.65 | 3.84 | 3650 | 3840 | 228 | 240 |
| Pyrophyllite | 2.84 | 2840 | 177 | ||||
| Pyrrhotite | 4.61 | 4610 | 288 | ||||
| Quartz | 2.62 | 2620 | 163 | ||||
| Rammelsbergite | 7.1 | 7100 | 443 | ||||
| Realgar | 3.56 | 3560 | 222 | ||||
| Rhodochrosite | Carbonate group | 3.69 | 3690 | 230 | |||
| Rhodonite | 3.5 | 3.7 | 3500 | 3700 | 218 | 231 | |
| Riebeckite | Amphibole group | 3.4 | 3400 | 212 | |||
| Roscoelite | Mica group | 2.97 | 2970 | 185 | |||
| Rutile | 4.25 | 4250 | 265 | ||||
| Samarskite | 5.6 | 5.8 | 5600 | 5800 | 349 | 362 | |
| Sanadine | 2.52 | 2520 | 157 | ||||
| Saponite | 2.3 | 2300 | 144 | ||||
| Scapolite | 2.66 | 2660 | 166 | ||||
| Scheelite | 6.01 | 6010 | 375 | ||||
| Scolecite | Zeolite group | 2.16 | 2.4 | 2160 | 2400 | 135 | 150 |
| Scorodite | 3.2 | 3200 | 200 | ||||
| Scorzalite | 3.27 | 3270 | 204 | ||||
| Semseyite | 5.8 | 6.1 | 5800 | 6100 | 362 | 381 | |
| Sepiolite | 2 | 2000 | 125 | ||||
| Serpentine | 2.53 | 2.65 | 2530 | 2650 | 158 | 165 | |
| Siderite | Carbonate group | 3.96 | 3960 | 247 | |||
| Siegenite | 4.9 | 4900 | 306 | ||||
| Sillimanite | 3.24 | 3240 | 202 | ||||
| Silver | 10.5 | 10500 | 655 | ||||
| Sklodowskite | 3.54 | 3540 | 221 | ||||
| Skutterudite | 6.1 | 6.9 | 6100 | 6900 | 381 | 431 | |
| Smithsonite | Carbonate group | 4.45 | 4450 | 278 | |||
| Soda nitre | 2.26 | 2260 | 141 | ||||
| Sodalite | Feldspathoid group | 2.29 | 2290 | 143 | |||
| Sperrylite | 10.58 | 10580 | 660 | ||||
| Spessartine | Garnet group | 4.18 | 4180 | 261 | |||
| Sphalerite | 4.05 | 4050 | 253 | ||||
| Sphene | 3.48 | 3480 | 217 | ||||
| Spinel group | 3.57 | 3.72 | 3570 | 3720 | 223 | 232 | |
| Spodumene | 3.15 | 3150 | 197 | ||||
| Stannite | 4.3 | 4.5 | 4300 | 4500 | 268 | 281 | |
| Staurolite | 3.71 | 3710 | 232 | ||||
| Stephanite | 6.25 | 6250 | 390 | ||||
| Sternbergite | 4.22 | 4220 | 263 | ||||
| Stibnite | 4.63 | 4630 | 289 | ||||
| Stilbite | Zeolite group | 2.15 | 2150 | 134 | |||
| Stillwellite | 4.61 | 4610 | 288 | ||||
| Stolzite | 7.9 | 8.2 | 7900 | 8200 | 493 | 512 | |
| Stromeyerite | 6 | 6.3 | 6000 | 6300 | 374 | 393 | |
| Strontianite | Carbonate group | 3.78 | 3780 | 236 | |||
| Sulphur | 2.06 | 2060 | 129 | ||||
| Sylvanite | 7.9 | 8.3 | 7900 | 8300 | 493 | 518 | |
| Sylvite | 1.99 | 1990 | 124 | ||||
| Talc | 2.75 | 2750 | 172 | ||||
| Tantalite | 6.2 | 8 | 6200 | 8000 | 387 | 499 | |
| Tennantite | 4.6 | 4.7 | 4600 | 4700 | 287 | 293 | |
| Tenorite | 6.5 | 6500 | 406 | ||||
| Tephroite | Olivine group | 4.11 | 4.39 | 4110 | 4390 | 256 | 274 |
| Tetrahedrite | 4.6 | 5.2 | 4600 | 5200 | 287 | 324 | |
| Thenardite | 2.68 | 2680 | 167 | ||||
| Thomsonite | Zeolite group | 2.34 | 2340 | 146 | |||
| Thorianite | 10 | 10000 | 624 | ||||
| Thorite | 4 | 6.7 | 4000 | 6700 | 250 | 418 | |
| Tin | 7.28 | 7280 | 454 | ||||
| Topaz | 3.55 | 3550 | 222 | ||||
| Torbernite | 3.2 | 3200 | 200 | ||||
| Tourmaline | 3 | 3.2 | 3000 | 3200 | 187 | 200 | |
| Tremolite | Amphibole group | 2.9 | 3.2 | 2900 | 3200 | 181 | 200 |
| Tridymite | 2.28 | 2.33 | 2280 | 2330 | 142 | 145 | |
| Triphylite | 3.4 | 3.6 | 3400 | 3600 | 212 | 225 | |
| Troilite | 4.61 | 4610 | 288 | ||||
| Trona | 2.13 | 2130 | 133 | ||||
| Tungstite | 5.5 | 5500 | 343 | ||||
| Turquoise | 2.6 | 2.8 | 2600 | 2800 | 162 | 175 | |
| Tyuyamunite | 3.3 | 4.3 | 3300 | 4300 | 206 | 268 | |
| Ulexite | 1.95 | 1950 | 122 | ||||
| Uraninite | 6.5 | 10.95 | 6500 | 10950 | 406 | 683 | |
| Uranophane | 3.9 | 3900 | 243 | ||||
| Uvarovite | Garnet group | 3.4 | 3.8 | 3400 | 3800 | 212 | 237 |
| Vanadinite | 6.8 | 7.1 | 6800 | 7100 | 424 | 443 | |
| Variscite | 2.5 | 2500 | 156 | ||||
| Vermiculite | Mica group | 2.3 | 2.5 | 2300 | 2500 | 144 | 156 |
| Violarite | 4.5 | 4.8 | 4500 | 4800 | 281 | 300 | |
| Vivianite | 2.65 | 2650 | 165 | ||||
| Wavellite | 2.34 | 2340 | 146 | ||||
| Willemite | 3.9 | 4.2 | 3900 | 4200 | 243 | 262 | |
| Witherite | Carbonate group | 4.3 | 4300 | 268 | |||
| Wolframite | 7.1 | 7.5 | 7100 | 7500 | 443 | 468 | |
| Wollastonite | 2.84 | 2840 | 177 | ||||
| Wulfenite | 6.5 | 7 | 6500 | 7000 | 406 | 437 | |
| Wurtzite | 4.03 | 4030 | 251 | ||||
| Xenotime | 4.4 | 5.1 | 4400 | 5100 | 275 | 318 | |
| Zincite | 5.43 | 5.7 | 5430 | 5700 | 339 | 356 | |
| Zinkenite | Jamesonite group | 5.12 | 5.35 | 5120 | 5350 | 319 | 334 |
| Zircon | 4.65 | 4650 | 290 | ||||
| Zoisite | 3.3 | 3300 | 206 | ||||
Related Topics
• Densities
Densities of solids, liquids and gases. Definitions and convertion calculators.
• Material Properties
Properties of gases, fluids and solids. Densities, specific heats, viscosities and more.
Related Documents
Bulk Modulus and Fluid Elasticities
Introduction to - and definition of - Bulk Modulus Elasticity commonly used to characterize the compressibility of fluids.
Concrete Mixtures
Cement, sand and gravel mixtures.
Density Converter
Online density converter with commonly used units.
Dirt and Mud - Densities
Densities - pound per cubic foot and kilograms per cubic metre - of dirt and mud.
Ditch Filling Materials - Densities
Weight or density of ditch filling materials.
Geological Time
Geological periods and time scale.
Liquid Densities
Densities of common liquids like acetone, beer, oil, water and more.
Liquids - Densities vs. Pressure and Temperature Change
Densities and specific volume of liquids vs. pressure and temperature change.
Malleability vs. Brittlenes vs. Ductility
Plastic deformation properties.
Metal Content in Minerals
Content of metals in minerals.
Mineral Hardness - Mohs Scale
The Mohs qualitative ordinal scale characterizes the scratch resistance of various minerals.
Mineral Wool Insulation
Thermal conductivity - k-values - vs. temperature.
Minerals and other Materials - Specific Gravities
Specific gravities for minerals and other materials.
Solids - Densities
Densities of selected solids.
Solids - Specific Heats
Common solids - like brick, cement, glass and many more - and their specific heats - in Imperial and SI units.
Stone Masonry - Strength
Typical strength of stone masonry constructions.
Stones - Weight and Strength
Weight and strength of sandstone, granite, limestone, marble and slate.
Storing Thermal Heat
Energy stored as sensible heat in different types of materials.