Carbon Steel Flanges - Group 1.1 Pressure and Temperature Ratings

Maximum temperature and pressure ratings of flanges conforming dimensions ASME B16.5 and materials specification ASTM A-105.

Pressure ratings for flanges conforming ASME B16.5 Pipe Flanges and Flanged Fittings - and materials specification ASTM A-105 Specification for Carbon Steel Forgings for Piping Applications - temperature in Fahrenheit and pressure in psi.

For full table - rotate the screen!

Carbon Steel Flanges - Group 1.1 Pressure and Temperature Ratings
Temperature (°C)
Working Pressure (bar)
Class
15030040060090015002500
-29 - 38 19.6 51.1 68.1 102.1 153.2 255.3 425.5
50 19.2 50.1 66.8 100.2 150.4 250.6 417.7
100 17.7 46.6 62.1 93.2 139.8 233.0 388.3
150 15.8 45.1 60.1 90.2 135.2 225.4 375.6
200 13.8 43.8 58.4 87.6 131.4 219.0 365.0
250 12.1 41.9 55.9 83.9 125.8 209.7 349.5
300 10.2 39.8 53.1 79.6 119.5 199.1 331.8
325 9.3 38.7 51.6 77.4 116.1 193.6 322.6
350 8.4 37.6 50.1 75.1 112.7 187.8 313.0
375 7.4 36.4 48.5 72.7 109.1 181.8 303.1
400 6.5 34.7 46.3 69.4 104.2 173.6 289.3
425 5.5 28.8 38.4 57.5 86.3 143.8 239.7
450 4.6 23.0 30.7 46.0 69.0 115.0 191.7
475 3.7 17.4 23.2 34.9 52.3 87.2 145.3
500 2.8 11.8 15.7 23.5 35.3 58.8 97.9
538 1.4 5.9 7.9 11.8 17.7 29.5 49.2

The values are for materials Group 1.1

  • 1 psi (lb/in2) = 144 psf (lbf/ft2) = 6,894.8 Pa (N/m2) = 6.895×10-3 N/mm2 = 6.895×10-2 bar
  • tC = 5/9 (tF - 32) 

Insert flanges to your Sketchup model with the Engineering ToolBox Sketchup Extension

Engineering ToolBox Sketchup Extension - flanges

3D Engineering ToolBox - draw and model technical applications! 2D Engineering ToolBox - create and share online diagram drawing templates! Engineering ToolBox Apps - mobile online and offline engineering applications!

Unit Converter


















































9.19.10

.
Cookie Settings