Rubbers and Elastomers - Chemical Resistance

Rsistance to chemicals - solvents and softeners - swelling properties.

Rubbers and elastomers resistance to chemicals, weathering, ultraviolet light and heat and temperature are indicated below. Solvents or softeneres and swelling properties are indicated too.

Rubbers and Elastomers - Chemical Resistance
Rubber or ElastomerChemical Resistant toSolvent or SoftenerSwelled by
Chemical NameCommercial Names
Polyisoprene Natural or Syntetic Rubber
NR, IR
Acetone
Acids
Alkalies
Alcohols
Carbon disulfide
Ketones
Petroleum products
Vegetable oils
Carbon disulfide
Petroleum products
Vegetable oils
Butadiene BR
Cis4
Glycerol
Glycol
Acids
Alkalies
Weathering
Aging
Carbon disulfide
Hexane
Turpentine
Petroleum products
Acetone
Petroleum products
Vegetable oils
Styrene-butadiene Buna S
Styrene
SBR
GR-S
Glycerol
Glycol
Acids
Alcohols
Salts
Oxidation
Ketones
Petroleum products
Aromatics
Vegetable oils
Petroleum products
Vegetable oils
Acrylonitrile butadiene Nitrile
Buna N
Hycar
NBR
GR-A
Glycerol
Glycol
Acids
Ketones
Alcohols
Petroleum products
Salts
Heat or high temperature
Vegetable oils
Weathering
Carbon tetrachloride
Ketones
Bitumen - coal derivates
Aromatics
Acetone
Phenol
Turpentine
Polychloroprene Neoprene
CR
GR-M
Glycerol
Glycol
Alcohols
Petroleum products
Salts
Heat or high temperature
Ultraviolet light
Vegetable oils
Weathering
Aging
Ozone
Acetone
Benzene
Carbon tetrachloride
Carbon disulfide
Acids
Turpentine
Aromatics
Carbon tetrachloride
Carbon disulfide
Turpentine
Aromatics
Isobutylene-isoprene Butyl
IIR
GR-I
Phenol
Glycerol
Glycol
Alkalies
Salts
Ultraviolet
Vegetable oils
Weathering
Oxidation
Aging
Ozone
Carbon disulfide
Petroleum products
Carbon disulfide
Hexane
Petroleum products
Polysulfide Thikol
PS
GR-P
Alcohols
Petroleum products
Ultraviolet light
Ozone
Carbon tetrachloride Carbon tetrachloride
Aromatics
Polymethane Adiprene
PU
Petroleum products
Vegetable oils
Oxidation
Ozone
  Benzene
Carbon tetrachloride
Ketones
Aromatics

Related Topics

  • Material Properties

    Properties of gases, fluids and solids. Densities, specific heats, viscosities and more.

Related Documents

Search

Search is the most efficient way to navigate the Engineering ToolBox.

Engineering ToolBox - SketchUp Extension - Online 3D modeling!

3D Engineering ToolBox Extension to SketchUp - add parametric components to your SketchUp model

Add standard and customized parametric components - like flange beams, lumbers, piping, stairs and more - to your Sketchup model with the Engineering ToolBox - SketchUp Extension - enabled for use with older versions of the amazing SketchUp Make and the newer "up to date" SketchUp Pro . Add the Engineering ToolBox extension to your SketchUp Make/Pro from the Extension Warehouse !

Translate this Page

Translate this page to Your Own Language .

About the Engineering ToolBox!

Privacy Policy

We don't collect information from our users. More about

We use a third-party to provide monetization technologies for our site. You can review their privacy and cookie policy here.

You can change your privacy settings by clicking the following button: .

Citation

This page can be cited as

  • The Engineering ToolBox (2008). Rubbers and Elastomers - Chemical Resistance. [online] Available at: https://www.engineeringtoolbox.com/chemical-resistance-rubbers-elastomers-d_1425.html [Accessed Day Month Year].